Post by Eugen »

I'm going to be plating some parts with zinc and thought I'd share the process with you guys. This is one of the easiest plating processes both in terms of procedure and ease of finding the necessary material. My source of information was an article written by Darlene Martin from Plating Resources Inc. I saved the article a while ago, and it's a good thing that I saved it because it appears to have disappeared from the internet, or at least I can't find it anymore.

The article covers multiple ways of doing zinc, nickel, and other metals, and a text version is attached here for your fun and delectation.

For me the easiest procedure was the alkaline formulation of the bath because it's the easiest to find the ingredients for the bath:
1. Distilled water (if you're a purist). I am guilty of using tap water once or twice. :D :109:
2. 40 g/liter Sodium carbonate. This is a fancy name for washing soda. Here in Canada you can find Arm & Hammer "So Clean" washing soda at Canadian Tire for about $5 a box. You can also make your own from baking soda. Put baking soda in a pan and heat it up while stirring continuously until it no longer bubbles.
3. 90 g/liter Sodium hydroxide. This is caustic soda, or lye. I found caustic soda crystals at home hardware, about $30 for a 2 liter jug. I used it in making my own soap and still have some around.
4. 1/2% per volume Addition agent. My understanding is that the addition agent ensures a bright plating, which I don't really care about. The quantity is also very small anyway.

The formulation calls for zinc metal, 15 g/liter.

In the past I have used a battery charger as source of current, set on the 2A setting. I'll show some pics when I start plating stuff.
electroplating-zinc.png

Anyway, join in the discussion if interested, it's not like I know this perfectly, but I have plated some parts successfully.
Attachments
electroplating.pdf
(67.96 KiB) Downloaded 117 times
Case 224, 444, 644, 680E
Kubota B26 :blush:
User avatar
Harry United States of America
Posts: 1510
Joined: Sun Mar 07, 2021 8:33 am
Location: Lockport,NY
Has thanked: 9362 times
Been thanked: 6333 times

Re: Zinc electroplating

Post by Harry »

Interesting post Eugen! I’m all ears to hear about the process. My only knowledge about plating was from a few welding repair jobs I did at a plating company. They did plating of many different metals and the acids used to clean the base metals were very caustic. This place was a cesspool to work at.I just did a few repair jobs for them and they were very happy with my work. They wanted me to come back but I had to turn them down because I didn’t want to get exposed to the chemicals in the air. :peace: Harry
1973 444, 1974 644, 1976 446, 1977 646, 1986 226
User avatar
RoamingGnome Canada
Posts: 639
Joined: Sun Jan 08, 2023 12:54 am
Location: Hamilton, ON
Has thanked: 9013 times
Been thanked: 3258 times

Re: Zinc electroplating

Post by RoamingGnome »

Interesting topic @Eugen Thanks for sharing...
'68 Case 195, '84 Case 446, '88 Ingersoll 222 - and 1965 Case 530ck (fullsize backhoe)
User avatar
DavidBarkey Canada
Posts: 3138
Joined: Sat Mar 06, 2021 10:35 am
Location: Waverley On.
Has thanked: 17253 times
Been thanked: 10585 times

Re: Zinc electroplating

Post by DavidBarkey »

Thats neat @Eugen . What is Addtion agent?
Dave
Mad Tractor Builder
User avatar
Eugen Canada
Posts: 5161
Joined: Wed Mar 03, 2021 2:52 pm
Location: Port Mcnicoll, Ontario
Has thanked: 12073 times
Been thanked: 16312 times
Contact:

Re: Zinc electroplating

Post by Eugen »

DavidBarkey wrote: Wed Apr 05, 2023 4:47 pm Thats neat @Eugen . What is Addtion agent?
Exactly I don't know.
I used once a little tsp and other times nothing.
Case 224, 444, 644, 680E
Kubota B26 :blush:
User avatar
Eugen Canada
Posts: 5161
Joined: Wed Mar 03, 2021 2:52 pm
Location: Port Mcnicoll, Ontario
Has thanked: 12073 times
Been thanked: 16312 times
Contact:

Re: Zinc electroplating

Post by Eugen »

Was going to do a little plating and can't find that lye. Where does the lye lie? I knew I had some left, but then again, maybe it's all gone.

So, plan B. Vinegar! That I got, plenty of. I try to always have a couple of gallons of that cheap vinegar around. And ammonia, but that's a different story. :violin:

There's another recipe like this: vinegar, water, and a fistful of salt. Vinegar, check. Water, check. Salt... just the pink joke from wherever in the world it comes from, 'cause I'm drat sure it's not from Himalaya. Let's experiment then, in a plastic container, add a gallon of vinegar, add a gallon of water, throw in a cup of washing soda (sodium carbonate). Let it finish bubbling, then two straps of zinc near each other in the bath, one on the positive one on the negative of the battery charger, on 2A limit. One of the zinc strips should show bubbling on its surface nearest the other strip. Let it go like that for about 40 minutes. The idea is that zinc will release into the bath ions, cat ions, or whatever they are called, my chemistry is not so good.
21A13294-660A-411D-93BB-71D1202F27AB.jpeg
Fine, now here are the parts I want to plate. See how I did not wire bush clean all of them perfectly. Unfortunately I did not have enough patience for that last night. This reminds me to build that parts shaker that it's been on the todo list for a million years.
548372D0-5539-4193-A42C-A22F78C22D8C.jpeg
String them on a wire, put them in the bath on the negative wire. The zinc electrodes/strips go on the positive. And let them bubble.
7F59B59B-FB18-4E40-A811-D54D097192BD.jpeg

Here they are after about 3 minutes.

E5A9B25E-52C6-483F-A043-6FAD90C2D5F5.jpeg

Notice how some areas are already plated, but others, which have not been cleaned well, are darker and not plated (yet?). I put them in and will let them go on for about 20 minutes, see if it made any difference to the dark areas. Stay tuned.


SAFETY WARNING: don't drink the chemical bath, don't let it jump into your eyes, wear gloves, wear glasses, wear a jacket, do this in open air and don't sniff the gases, because I have no idea if the fumes are flammable or bad for your lungs. Better yet, don't do it because I don't know if it's dangerous. If you do it and you get hurt or you burn your house it's not my fault. :107:
Case 224, 444, 644, 680E
Kubota B26 :blush:
User avatar
RoamingGnome Canada
Posts: 639
Joined: Sun Jan 08, 2023 12:54 am
Location: Hamilton, ON
Has thanked: 9013 times
Been thanked: 3258 times

Re: Zinc electroplating

Post by RoamingGnome »

Eugen wrote: Thu Apr 06, 2023 12:07 pm
SAFETY WARNING: don't drink the chemical bath, don't let it jump into your eyes, wear gloves, wear glasses, wear a jacket, do this in open air and don't sniff the gases, because I have no idea if the fumes are flammable or bad for your lungs. Better yet, don't do it because I don't know if it's dangerous. If you do it and you get hurt or you burn your house it's not my fault. :107:
"Don't drink the chemical bath..." :rofl: :rofl: :rofl:

We need to find you one of those kids chemistry sets from the '50s and 60's... don't know how my generation survived :))
'68 Case 195, '84 Case 446, '88 Ingersoll 222 - and 1965 Case 530ck (fullsize backhoe)
User avatar
Eugen Canada
Posts: 5161
Joined: Wed Mar 03, 2021 2:52 pm
Location: Port Mcnicoll, Ontario
Has thanked: 12073 times
Been thanked: 16312 times
Contact:

Re: Zinc electroplating

Post by Eugen »

@RoamingGnome :rofl: :rofl:


Ok, so the experiment continues. The parts that were not exactly cleaned well of rust went back in the plating bath for about 1.5 hours.

This is the result.

One not rubbed the other two with some rubbing for shine. :D

I declare the experiment a succes.
F52E8E6B-9065-4E13-A015-6BB61E33AC75.jpeg
155DFF05-1D6A-4AD4-B05B-5AD9AE7163B8.jpeg
04CD26E5-6D82-458A-83F0-5F87BFABE85C.jpeg
Case 224, 444, 644, 680E
Kubota B26 :blush:
User avatar
DavidBarkey Canada
Posts: 3138
Joined: Sat Mar 06, 2021 10:35 am
Location: Waverley On.
Has thanked: 17253 times
Been thanked: 10585 times

Re: Zinc electroplating

Post by DavidBarkey »

RoamingGnome wrote: Thu Apr 06, 2023 12:42 pm
Eugen wrote: Thu Apr 06, 2023 12:07 pm
SAFETY WARNING: don't drink the chemical bath, don't let it jump into your eyes, wear gloves, wear glasses, wear a jacket, do this in open air and don't sniff the gases, because I have no idea if the fumes are flammable or bad for your lungs. Better yet, don't do it because I don't know if it's dangerous. If you do it and you get hurt or you burn your house it's not my fault. :107:
"Don't drink the chemical bath..." :rofl: :rofl: :rofl:

We need to find you one of those kids chemistry sets from the '50s and 60's... don't know how my generation survived :))
Natural selection . The dumb ones didn't make it .
Dave
Mad Tractor Builder
User avatar
Eugen Canada
Posts: 5161
Joined: Wed Mar 03, 2021 2:52 pm
Location: Port Mcnicoll, Ontario
Has thanked: 12073 times
Been thanked: 16312 times
Contact:

Re: Zinc electroplating

Post by Eugen »

Comparison. Zinc plated and wire brushed vs the old state still to be done. The zinc layer is thick enough to take a good brush on.

003845C5-8024-4465-AB3E-DE2577E54906.jpeg
Case 224, 444, 644, 680E
Kubota B26 :blush:
Post Reply